Pick the metal, thickness and process. You get starting amps, wire feed speed and voltage for MIG and flux-core, rod size for stick, and tungsten and amps for TIG, based on published maker charts and the 1 amp per 0.001 inch rule. These are starting points: test on scrap and follow your machine's door chart.
Affiliate disclosure: as an Amazon Associate, CanItBeWelded.com earns from qualifying purchases, at no extra cost to you. These links are searches, not endorsements of a specific product.
How the starting points are worked out
- Target amps. About 1 amp per 0.001 in of thickness. It picks the wire or rod size whose published range covers that amperage.
- MIG and flux-core. Wire feed speed and voltage come from Lincoln Electric's published typical operating procedures for the wire. Between two published rows, values are interpolated in a straight line by amps. Outside a wire's published range, the nearest published point is shown with a warning.
- Stick. The smallest rod whose published current range includes the target amps, plus the next size down for comparison. Ranges are from Lincoln's electrode data.
- TIG. Amp ranges, tungsten, cup and gas flow are from Miller's TIG settings ranges as compiled by Welding Tribe, matched to the nearest published thickness. The compilation is a secondary source, so confirm against Miller's calculator.
- Polarity. Every result lists polarity. DC+ (electrode positive, also called DCEP) and DC− (electrode negative, DCEN) are shown as the makers publish them. Stick and TIG are set by amps, so they have no voltage or wire-speed dial.
- Not covered. Flux-core on stainless and aluminum, and stick on aluminum. The calculator says so instead of guessing.
Example: 1/8 in mild steel
| Process | Wire or rod | Starting point |
|---|---|---|
| MIG solid wire, mild steel | ER70S-6 solid wire (AWS A5.18) | 0.030 in short circuit: about 288 in/min, 19.7 to 20.7 V (DC+) 0.035 in short circuit: about 159 in/min, 17.3 to 18.3 V (DC+) |
| Flux-core, self-shielded | E71T-11 self-shielded flux-core (Lincoln Innershield NR-211-MP) | 0.030 in: about 242 in/min, 14.8 to 15.8 V (DC−) |
| Flux-core, gas-shielded | E71T-1 gas-shielded flux-core (Lincoln UltraCore 71A85) | 0.045 in: about 175 in/min, 21 to 26 V (DC+) |
| Stick | E6011 (Lincoln Fleetweld 180) | 5/32 in, start about 125 A (published DC range 105 to 135 A) |
| Stick | E6013 (Lincoln Fleetweld 37) | 1/8 in, start about 125 A (published DC range 100 to 135 A) |
| Stick | E7018 (Lincoln Excalibur 7018 MR) | 1/8 in, start about 125 A (published DC range 90 to 160 A) |
| TIG, butt joint | ER70S-2 | 95 to 130 A, tungsten 1/16 in (Miller) or 3/32 in (Lincoln), DCEN (electrode negative) |
MIG voltages above use the 75/25 adjustment. Pick 100% CO2 in the calculator for the CO2 table values.
Target amps by thickness
| Thickness | 1 A per 0.001 in |
|---|---|
| 0.024 in (24 ga steel) | 24 A |
| 0.030 in (22 ga steel) | 30 A |
| 0.036 in (20 ga steel) | 36 A |
| 0.048 in (18 ga steel) | 48 A |
| 0.060 in (16 ga steel) | 60 A |
| 0.075 in (14 ga steel) | 75 A |
| 0.105 in (12 ga steel) | 105 A |
| 1/8 in (0.125) | 125 A |
| 3/16 in (0.1875) | 188 A |
| 1/4 in (0.250) | 250 A |
| 3/8 in (0.375) | 375 A |
| 1/2 in (0.500) | 500 A |
Published stick electrode ranges
| Electrode | Rod | DC amps | AC amps |
|---|---|---|---|
| E6011 (Lincoln Fleetweld 180) | 3/32 in | 40 to 80 | 40 to 90 |
| E6011 (Lincoln Fleetweld 180) | 1/8 in | 60 to 110 | 65 to 120 |
| E6011 (Lincoln Fleetweld 180) | 5/32 in | 105 to 135 | 115 to 150 |
| E6013 (Lincoln Fleetweld 37) | 1/16 in | 20 to 45 | 20 to 45 |
| E6013 (Lincoln Fleetweld 37) | 5/64 in | 45 to 75 | 50 to 80 |
| E6013 (Lincoln Fleetweld 37) | 3/32 in | 70 to 105 | 75 to 115 |
| E6013 (Lincoln Fleetweld 37) | 1/8 in | 100 to 135 | 110 to 140 |
| E6013 (Lincoln Fleetweld 37) | 5/32 in | 145 to 180 | 160 to 200 |
| E6013 (Lincoln Fleetweld 37) | 3/16 in | 185 to 235 | 205 to 260 |
| E7018 (Lincoln Excalibur 7018 MR) | 3/32 in | 70 to 110 | 80 to 120 |
| E7018 (Lincoln Excalibur 7018 MR) | 1/8 in | 90 to 160 | 100 to 160 |
| E7018 (Lincoln Excalibur 7018 MR) | 5/32 in | 130 to 210 | 140 to 210 |
| E7018 (Lincoln Excalibur 7018 MR) | 3/16 in | 180 to 300 | 200 to 300 |
| E7018 (Lincoln Excalibur 7018 MR) | 7/32 in | 250 to 330 | 270 to 370 |
| E7018 (Lincoln Excalibur 7018 MR) | 1/4 in | 300 to 400 | 325 to 420 |
| E308L-16 (Lincoln Arosta 304L) for 304/304L | 3/32 in | 40 to 70 | · |
| E308L-16 (Lincoln Arosta 304L) for 304/304L | 1/8 in | 60 to 110 | · |
| E308L-16 (Lincoln Arosta 304L) for 304/304L | 5/32 in | 80 to 150 | · |
Sources
- Lincoln Electric SuperArc L-56 (ER70S-6), Typical Operating Procedures
- Lincoln Electric Red Max 308LSi, Typical Operating Procedures
- Lincoln Electric SuperGlaze 4043 and SuperGlaze 5356, Typical Operating Procedures
- Lincoln Electric Innershield NR-211-MP (E71T-11), Typical Operating Procedures
- Lincoln Electric UltraCore 71A85 (E71T-1), Typical Operating Procedures
- Lincoln Electric Fleetweld 180 (E6011), Fleetweld 37 (E6013), Excalibur 7018 MR (E7018): Typical Operating Procedures; Arosta 304L (E308L-16); 1/16 in E6013 range from Lincoln C2.410
- Miller TIG welding calculator and Guide to TIG Welding Basics; Lincoln Square Wave TIG 200 guide (L16988); ranges as compiled by Welding Tribe (Nov 2026)
- Welding Tribe TIG settings chart (Miller and Lincoln ranges)
Related guides and tools
Frequently asked questions
What amperage should I use to weld 1/8 inch steel?
A common starting rule is about 1 amp per 0.001 in of thickness, so 1/8 in (0.125 in) starts near 125 A. In Lincoln's published charts that is 0.030 in or 0.035 in solid wire for MIG, a 1/8 in E7018 or E6013 rod for stick (E7018 published DC range 90 to 160 A), and the Miller TIG range of 95 to 130 A on a butt joint. Treat every figure as a starting point and test on scrap.
What is the 1 amp per 0.001 inch rule?
A rule of thumb for steel: set the amperage to about 1 amp for every 0.001 in of metal thickness, then adjust for process, joint, position and your machine. It is only a starting point, which is why this calculator also uses the published wire and rod tables.
What wire size do I use for thin sheet metal with a MIG welder?
Lincoln publishes 0.025 in wire for roughly 35 to 80 A and 0.030 in wire for roughly 35 to 130 A (short-circuit transfer). The smaller wire runs cooler, which helps on sheet. Below about 35 A, the published charts stop, so go by your machine's sheet-metal setting.
What polarity does flux-core wire use?
It depends on the wire. Self-shielded flux-core (E71T-11, such as Lincoln Innershield NR-211-MP) runs on DC electrode negative. Gas-shielded flux-core (E71T-1, such as Lincoln UltraCore 71A85) runs on DC electrode positive with an Ar/CO2 mix. Check the wire's spool label.
Do I change the voltage for 75/25 gas instead of CO2?
Lincoln's short-circuit MIG settings are given for CO2. With 75% argon / 25% CO2, Lincoln says to lower the voltage 1 to 2 V. The calculator applies that adjustment when you pick the mix.
Which settings win, this calculator or the chart inside my welder?
The chart on your welder's door or in its manual wins. This calculator uses published maker starting points for typical equipment, and your machine, wire brand, stickout, joint and position can all shift them.
Can I use it for aluminum?
For TIG, yes: the Miller ranges are listed with AC polarity and argon, and you need an AC-capable machine. For MIG, Lincoln publishes only a few typical points at 170 A and up, so thinner aluminum needs a spool gun or pulse program and your machine's aluminum chart.