Home › Guides › Metals & Welding Basics › When to preheat before welding
When to Preheat Before Welding (and How to Do It Right)
From CanItBeWelded.com, run by Rick, a working welder at RickTheWelder. Published November 29, 2026. How we write and check guides.
Quick answer
- Preheat slows cooling. Slower cooling means less hard, brittle metal next to the weld, less trapped hydrogen, and less shrinkage stress. That is what prevents cracking.
- Almost always preheat: cast iron, thick sections of carbon steel, high-carbon and alloy steels such as hardened parts and thick chromoly, and any metal that is below freezing.
- Often helpful: thick aluminum and copper, which pull heat away so fast that the start of the weld will not fuse.
- Usually not needed: thin mild steel in a warm shop.
- Measure it. Temperature crayons or a thermometer, not a guess, and heat a wide area evenly. Then cool slowly when the part calls for it.
What preheat actually does
When a weld cools, the metal next to it, called the heat-affected zone, cools very quickly because the cold part around it soaks heat away. In steels with more carbon or alloy, fast cooling makes that zone hard and brittle. Hydrogen from moisture, rust, oil or damp rod gets trapped in that hard zone and can cause cracks hours after welding, often called hydrogen or delayed cracking. In cast iron, uneven heating and cooling causes shrinkage cracks right next to the bead.
Preheating the part before welding slows that cooling, drives off moisture, and spreads out the thermal stress. It is one of the cheapest ways to prevent a repair from cracking.
Jobs that need preheat
- Cast iron: nearly always. Many cast iron welders heat the whole casting evenly, to several hundred degrees Fahrenheit, for the hot method. Others use a cold method with nickel rod, short beads and peening. Either way, uneven heat is the enemy. See cast iron.
- Thick carbon steel: as thickness goes up, the part pulls heat away faster. Heavy plate, thick hitch tongues, equipment buckets and frame rails often call for preheat, especially when the joint is restrained from both sides.
- Higher-carbon and alloy steel: springs, blades, axle shafts, hardened pins, tool steel and thick 4130 chromoly. These are the steels most prone to cracking. See hardened steel and chromoly.
- Unknown steel on a heavy part: if you cannot identify the grade and the part is thick, preheating is a sensible precaution.
- Cold weather: metal that is below freezing or wet with frost should at least be warmed until it is dry and warm to the touch before welding. See welding in rain and cold.
- Thick aluminum and copper: these conduct heat away so well that the arc cannot form a puddle at the start. Preheat helps the weld fuse instead of sitting cold on top.
How hot? Follow the maker, not a rumor
The right preheat depends on the exact steel or casting, its thickness, how restrained the joint is, and the filler. Structural welding codes and filler makers publish preheat tables based on these, and the steel's carbon equivalent, a number that combines carbon and alloy content, is the main input. For repair work on an unknown part, welders tend to use conservative preheat and low-hydrogen filler on anything thick or hard. If you know the alloy, use the filler or steel maker's recommendation. The point to remember is that too little preheat risks cracks, and too much can damage heat-treated parts.
How to preheat
- Heat broad, not hot spots. A rosebud tip on an oxy-fuel torch, a propane burner for large parts, an oven for small castings, or induction heating in a shop. Heat several inches on each side of the joint, and the whole casting when it is cast iron.
- Heat from the far side when you can so the surface you will weld does not overheat while the core is still cold.
- Measure. Temperature-indicating crayons melt at a marked temperature and are cheap and reliable. Contact thermometers work too. Infrared thermometers are handy but can read wrong on shiny metal.
- Hold interpass temperature. On multi-pass repairs, the part should not cool below the preheat between passes, and should not climb too high either.
- Cool slowly when needed. Cast iron and hardenable steels benefit from slow cooling: wrap the part in a welding blanket, bury it in dry sand or vermiculite, or let a stove or oven cool down with the part inside.
When preheat hurts
- Heat-treated aluminum such as 6061-T6 loses strength when heated, so preheating it hot for a long time can make things worse. Use only enough to drive off moisture or to start the puddle on thick parts.
- Thin sheet warps and burns through more easily if preheated.
- Parts near seals, bearings, wiring, fuel lines or paint can be damaged by broad heat. Remove them first.
- Coated or painted parts give off heavy fumes when heated. Strip the area and ventilate.
Low-hydrogen practice goes with preheat
Preheat works best alongside other habits that keep hydrogen out of the weld: clean the joint of rust, oil and paint, use low-hydrogen rods such as E7018 stored dry, keep wire and rod out of damp air, and never weld on wet or frosted metal. Our rod and wire guide covers which fillers are low hydrogen.
Need starting amps for a thick part after preheat? Use the Welding Settings Calculator.
🧰 Tools & parts for this job
The links in the strip at the top of this page are Amazon searches for the gear this job uses. They are paid links (Amazon Associate), not endorsements of a specific product. Links never change a verdict.
⚠️ Safety
- Preheated parts stay dangerously hot for a long time. Mark them as hot and keep people away.
- Large torch flames reach farther than you expect. Clear flammables and check for smoldering material afterward.
- Do not preheat any closed container, tank or hollow part that could hold liquid or vapor.
- Heating painted, galvanized or oily parts makes toxic smoke. Strip coatings and ventilate.
Common questions
Do I need to preheat mild steel?
Thin mild steel in a warm shop usually does not need preheat. Thick sections, highly restrained joints, cold or damp parts, and repairs on unknown steel often benefit from it.
How do I know how hot the part is?
Temperature-indicating crayons are the simplest: mark the metal and the mark melts when it reaches the crayon's temperature. Contact thermometers also work. Infrared thermometers can misread shiny metal.
Why do welds crack hours later?
Often hydrogen cracking: hydrogen from moisture, rust, oil or damp rod trapped in hard metal next to the weld. Preheat, clean metal and low-hydrogen filler help prevent it.
Should I preheat cast iron?
In most cases, yes, evenly across the casting, and then cool it slowly. Some welders use a cold method with nickel rod and very short beads instead, but uneven heat is always the main cause of cracking.
Can I preheat with a propane torch?
For small parts, a propane torch can work. For thick or large parts, a rosebud tip on an oxy-fuel torch or a large propane burner heats more evenly and faster.