- Porosity (pinholes): gas trapped in the weld from rust, paint, oil, moisture, or shielding gas blown away by wind.
- Lack of fusion and cold lap: the bead sits on top instead of melting in. Too little heat, too fast, or the wrong angle. Looks fine, breaks easily.
- Cracking: in the weld centerline or crater from shrinkage and the wrong filler, or beside the weld from hard, hydrogen-loaded metal that needed preheat.
- Fatigue: a sound weld placed at a sharp corner or ending at a stress point can crack after months of vibration.
- Most defects are prevented by prep: bright clean metal, correct settings, proper fit-up, the right filler and preheat when the metal needs it.
How to read a failed weld
When a repair fails, the break itself tells you a lot. Look at where it broke (through the weld, along its edge, or in the metal beside it), what the broken face looks like, and how long the repair lasted. A weld that peeled off cleanly with smooth, unmelted metal underneath never fused. A break through the middle of the bead points to a weak or cracked weld. A crack in the metal beside the weld points to hard, brittle heat-affected metal or fatigue. A failure after months of use with rust staining on part of the break is classic fatigue.
Porosity
What it looks like: pinholes on the surface or bubbles inside the weld when it is ground or cut.
Causes: rust, paint, oil, galvanizing, moisture or mill scale in the joint; shielding gas blown away by wind or a fan; an empty or leaking gas bottle; a dirty nozzle; damp flux-core wire or stick rod; aluminum oxide and moisture on aluminum.
Prevention: clean to bright metal, check gas flow and hoses, block wind or switch to stick or self-shielded flux-core outdoors, and keep filler dry. Porous welds should be ground out and rewelded, not covered over.
Lack of fusion, cold lap and poor penetration
What it looks like: a tall, ropey bead with edges that sit on the surface without blending in, or a weld that looks good on top but did not reach the root of the joint. On a broken part, you see smooth original metal under the weld.
Causes: too little amperage or voltage for the thickness, travel speed too fast, wrong gun or rod angle, a small machine on thick steel, no bevel on thick material, or welding over a gap that was too tight.
Prevention: set the machine for the thickness, bevel thick joints and use several passes, leave the right root gap, and test on scrap of the same thickness. Cut a test weld and look at the cross section, or break it in a vise. This defect is the most dangerous because it hides behind a nice-looking bead. See Can a small welder weld thick steel?
Undercut, overlap and burn-through
- Undercut: a groove melted into the base metal along the edge of the weld and left unfilled. It thins the part right at a stress point. Usually from too much heat, too long an arc, or the wrong angle.
- Overlap: weld metal that rolls over onto the base metal without fusing. Usually too cold or too slow.
- Burn-through: holes melted through thin metal. Use less heat, smaller wire, short stitches and a backing bar. See thin sheet metal.
Slag inclusions
Stick and flux-core welds leave slag on top. If it is not chipped and brushed off completely between passes, it gets trapped in the next pass as a weak spot. Clean each pass, grind out any trapped slag, and avoid welding into tight grooves where slag cannot float out.
Cracks in the weld itself
- Crater cracks: small star or line cracks at the end of a bead where the puddle shrank as it froze. Fill the crater by pausing or backstepping before breaking the arc.
- Centerline (hot) cracks: a crack down the middle of the bead as it solidifies. Common with a deep, narrow bead, high-sulfur or high-carbon steel, the wrong aluminum filler, or a joint under heavy restraint. Change the bead shape, the filler or the joint design.
- Aluminum cracking: some aluminum alloys crack with the wrong filler. 4043 and 5356 are not interchangeable on every alloy. See the rod and wire guide.
Cracks beside the weld (heat-affected zone)
When steel with more carbon or alloy cools quickly after welding, the metal next to the weld turns hard and brittle. Add hydrogen from moisture, rust or damp rod and you can get cracks that appear hours after welding. Cast iron behaves the same way, only worse. Prevention is preheat, low-hydrogen filler, clean metal and slow cooling, covered in when to preheat. On cast iron, nickel rod or brazing helps; see cast iron.
Fatigue: the weld was fine, the design was not
Many repair welds fail months later even though the welding was good. Vibration and repeated loads concentrate at sharp changes in shape: the toe of a fillet weld, the end of a weld, a hole, a notch or a stiff gusset that ends abruptly. Trailer frames, mower decks, loader arms and hitches are full of these spots.
- Do not start or stop welds at the highest stress point. Wrap around corners where possible.
- Taper or round the ends of reinforcing plates and gussets so stress spreads out.
- Grind cracks out completely, including both ends, before welding. Drilling a small hole at each end stops a crack from running while you work.
- Find the cause: overload, a missing brace, or a loose bolt that let a part flex.
The trailer frame crack guide shows a reinforcing plate used this way.
How welders check their work
- Visual inspection: even width, edges blended in, no undercut, no pinholes, crater filled.
- Break and cut tests on scrap: weld two coupons the same way and break them or cut them to see penetration.
- Dye penetrant: an inexpensive spray kit that shows surface cracks on any metal.
- Professional methods: magnetic particle, ultrasonic and X-ray testing are used by inspection companies on critical work.
Settings that are too cold cause many of these defects. Get starting points from the Welding Settings Calculator.
🧰 Tools & parts for this job
The links in the strip at the top of this page are Amazon searches for the gear this job uses. They are paid links (Amazon Associate), not endorsements of a specific product. Links never change a verdict.
⚠️ Safety
- A weld that has failed once on a safety part should be inspected by a qualified welder before the part is used again.
- Grinding out old welds throws sparks and fragments. Wear a face shield and keep flammables away.
- Never use chlorinated brake cleaner to degrease before welding. Heat and arc light can turn its vapor into toxic phosgene gas. Use acetone or a non-chlorinated cleaner and let it dry.
- Dye penetrant sprays are flammable. Use them only on cold parts, away from the arc.
Common questions
Why does my weld look good but break?
Usually lack of fusion or poor penetration: the bead sat on top of the metal without melting into it. It is common with a small machine on thick steel or travel speed that is too fast. Cut or break a test weld to check.
What causes holes in a weld?
Porosity, from contamination such as rust, paint, oil or moisture, or from shielding gas being blown away or not flowing. Clean the joint, check the gas, and block wind.
Why did my weld crack the next day?
Delayed cracking is often hydrogen cracking in hard metal next to the weld, common on thick, high-carbon or alloy steel welded without preheat or with damp filler.
Can you weld over a cracked weld?
Not directly. Grind the crack out completely to sound metal, find out why it cracked, then reweld. Welding over a crack usually leaves the crack inside the new weld.
How do I stop a crack from spreading before I weld it?
Find both ends with dye penetrant or a magnifier and drill a small hole just past each end. Then grind out the crack and weld.